Pre-treatment
If the surface finish of the MDF ex-works does not meet the quality requiremens of the end product, the surface has to be sanded. This will ensure that the material has an evenly smooth surface and is free of any contaminants, minor scratches, dust, grease, etc. For more information, see IGP-TI 111.
Coating devices
All conventional electrostatic systems with corona charging.
For the construction and operation of powder coating plants, the following regulations must be complied with: ATEX RL 2014/34/EU, EN 50177, DIN EN 16985.
Curing conditions
TObject | t min | t max |
---|
125 °C | 10 minutes | 15 minutes |
135 °C | 5 minutes | 10 minutes |
150 °C | 3 minutes | 5 minutes |
Due to the limited thermal conductivity, the use of infrared- (electric / gas catalytic) or convectional - infrared combined ovens is recommended.
In order to determine ideal curing conditions, we recommend practical trials with the respective object and curing oven.
The curing conditions must be carefully controlled. Powder coatings cured outside the curing window may show deficiencies in the film flexibility. Our technical customer service will advise you.
Reclaimability
Small portions of recycled powder can be added, automatically if possible, to the fresh powder. Important: Keep overspray to an absolute minimum.